Indium Seals

Due to its softness and compressibility, indium is ideal for use in creating a seal.

Let's get right into it:

Indium preforms are commonly used to create seals. The preforms are made into an endless variety of shapes and sizes to fit the application. Crucial to the seal is the thickness of the preform, because, if the volume of indium is insufficient, the seal will eventually fail – due to lack of indium to fill in the gaps.

Indium wire is also a form used in the creation of a vacuum, hermetic or cryogenic seal. Care must be taken to insure that the correct diameter of wire is used to make the seal. Too small of a diameter, the gap will not be adequately filled leaving the seal area vulnerable to leaks. Too large, and the indium, when compressed, will exit the seal area and may interfere with other electronics in the area.

When using wire, care must be taken to have the wire centered in the area to be sealed. If the wire is off-centered, it may not create an adequate seal when compressed due to non-uniformity. In some cases, it is beneficial to make a small groove in the seal area so the wire can be placed using the groove as a guide for accurate placement.

Indium metal is self-passivating and will form about 80-100 Angstroms of oxide on its surface at room temperature. In more critical seal applications, it is essential that this oxide layer be removed prior to creating the seal because if the oxide is present during the compression of the indium, the oxide will be pushed below the surface and could create a path for leakage.

Not all seals require the same level of performance. A purity of 99.99% indium is adequate for a vacuum, hermetic or cryogenic seal, but higher purities are also available if needed. Some seals need to maintain their integrity for many years while others only need to hold for a short period of time. Develop your design based on what you know about the application.The more critical seals will need to be made following the procedure outlined below to insure that the integrity requirements are met.

  • Degrease the indium in acetone to remove any surface organics that could interfere with the seal.
  • Place the indium in 10% HCl for about 1 minute to remove the oxide on the surface.
  • Rinse thoroughly in DI water to remove the HCl.
  • Rinse in acetone to remove the water.
  • Blow dry with dry nitrogen or allow to air dry.

Please see our Application Note on Etching Indium to Remove Oxides, and watch this video to see how it's done.

Caution:

Indium will cold weld to itself, especially after the surface oxides have been removed. See exactly what I mean. Care must be taken that the indium is not allowed to touch other freshly etched pieces of indium, as they will stick together similar to Contact Cement. Separation is difficult, if not impossible, without damaging the indium piece.

Please see our Application Note on the Cold Welding of Indium.

After the indium is ready to use, care must be taken in the proper placement of the preform or wire on the surface to be sealed. Once the indium is in place, the amount of pressure required to make the seal is dependent on the application. A few trials may be required until just the right amount of pressure is determined to form the seal that is needed. These trials are also a good time for adjustments to be made in the thickness of the indium used.

Feel free to tap into our experience and knowledge to help you shorten the time to get your seal process ready for implementation.