Skip to content

Tin Whiskers 101: Part 2: What Causes Them

Folks,

Continuing our series on tin whiskers. In the last post we discussed what they are. in this post we will discuss what causes them.

Tin whiskers are primarily caused by compressive stresses in tin. The most common cause of the stresses is copper diffusion into the tin as seen in Figure 1a. Such diffusion is common when tin is plated, melted or evaporated on copper. Copper preferentially diffuses into tin exacerbating tin whisker production.

Four-panel diagram showing tin whisker formation under thermal cycling, corrosion, and mechanical.

Figure 1. Some causes of tin whiskers

Another cause of tin whiskers can occur when the tin is plated, melted or evaporated on a material that has a lower coefficient of expansion than the tin, such as alloy 42 or ceramic. When temperature increases, the tin is constrained by the lower coefficient of expansion material. This constraint causes compressive stresses in the tin that can result in tin whiskers. See Figure 1b.

Less common causes are corrosion, as seen in Figure 1c and mechanical stresses as seen in Figure 1d.

Since copper diffusion is one of the most likely causes of tin whiskers, this mechanism deserves elaboration. The left image in Figure 2 depicts the mechanism of copper diffusion into tin. The mechanism is so strong that the diffusion of the copper often leaves voids in the copper. Such voids are called Kirkendall voids. The right image in Figure 2 is an x-ray map of copper (green) diffusing into the tin (black).

Cross-section diagram of a Sn layer over CuSn and Cu with a Kirkendall void, beside an EDS map.

Figure 2. Copper diffusing into tin.

Clearly, one way to minimize this type of tin whisker growth is to prevent copper diffusing into tin. In a future post, we will discuss this and other tin whisker mitigation techniques.

Cheers,

Dr. Ron