New Excel Software Tools to Practice for SMTA Certification #2: Reflow Profiling

Folks,

In my last post, I shared about an Excel®-based software toolcalled Line Balancer™to help candidates for SMTA Certification prepare for the line balancing part of the program. They can use Line Balancer™ to check the correctness of practice line balancing problems. This post will discuss another Excel®-based software tool, Reflow Profiler™, to help candidates prep for the reflow profiling part of the certification.

Typically, the reflow profiling goal is to determine if the reflow profile matches the requirements of the solder paste specification.

As an example, let’s consider a reflow profile as shown in Figure 1. The solder paste specification is shown in Figure 2. We will first solve the problem by hand and then use the software.

Reflow temperature profile graph showing temperature in °C versus time in seconds, peaking near.

Figure 1. A ramp-to-peak reflow profile.

Table of SAC305 reflow profile parameters, listing recommended and acceptable ranges for ramp.

Figure 2. The solder paste reflow specification

The first task is to determine if the ramp-to-peak rate matches the solder paste specification outlined in red in the specification shown in Figure 3. By measuring the change in temperature in Figure 4 from point A to B and dividing it by the change in time from those points, we see in Figure 4 that the ramp-to peak-rate is 0.857 C/seconds, and is within therecommended specifications 0.5 to 1.0 C/second.

Table of SAC305 reflow profile parameters, comparing recommended and acceptable ranges for ramp.

Figure 3. The solder paste specification with the ramp-to-peak rate highlighted.

Line graph of a reflow temperature profile plotting temperature in °C against time in seconds.

Figure 4. The reflow profile with the ramp-to-peak rate calculated.

Figure 5 shows the solder paste specification with the time above liquidus (TAL) with the peak temperature highlighted. While Figure 6 shows the reflow profile, where the TAL is measured as 60 seconds and the peak temperature at 240C, both are consistent with the recommended values.

Table of SAC305 reflow profile parameters, comparing recommended and acceptable ranges for ramp.

Figure 5. The solder paste specification with the TAL and peak temperature highlighted.

Reflow profile graph showing 60-second TAL between 230°C and 290°C with a 240°C peak temperature.

Figure 6. The reflow profile with the TAL and peak temperature identified.

Lastly, Figure 7 shows the solder paste specification with the cooling ramp rate highlighted and Figure 8 shows the reflow profile with the cooling rate calculated as -2.8 C/s, again within the specification.

Table of SAC305 reflow profile recommended and acceptable parameters, including ramp, soak, TAL.

Figure 7. The solder paste specification with the cooling rate highlighted.

A reflow temperature profile graph plotting temperature in °C against time in seconds, with points.

Figure 8. The reflow profile with the cooling rate calculated.

Spreadsheet screenshot with colored data tables, a line graph, and a small logo in the lower right.

Figure 9 shows all of the calculations performed and matched to the specification with Reflow Profiler™.

If you are interested in a copy of Reflow Profiler™, send me an email at [email protected].

Cheers,
Dr. Ron