Gold-Tin Eutectic Solder

Gold tin eutectic solder (AuSn20, or 80%gold, 20%tin by weight) isused in a varietyof applications requiring ahigh reliability, high melting solder joint. This includes die-attach and even lid-attach for hermetically-sealed ceramic packages. When usedas adie-attach solder alloy for LED or RF GaN devices, voiding becomes a critical issue. Die in these applications have to be able to pass very high currents (at very high currentdensities, due to the low die area), yet for maximum device lifetime and maximum efficiency, they must be maintainedat as low a temperature as possible. This is only feasible if the heat energy at the die surfacecan be removed efficiently (minimizing Tj), meaning that theheat transfer between the die and leadframe (or submount) must bemaximized. There are three well-known ways to achieve this:

  1. Increase the thermal conductivity (K) of the die-attach material
  2. Reduce the bondline thickness (BLT)between the die and leadframe
  3. Minimize voiding

Note that there is frequently a tradeoff between 2 and 3, in that minimizing the BLT can increase voiding, so, pragmatically, a minimum of around 10 microns (0.4 mil) is most commonly used. A smaller BLT also has the effect, often neglected, of making the contribution of gold-metallized soldering surfaces on both the die and submount non-trivial, so skewingthe alloy away from the ideal eutectic.The details of the gold-tin phase diagram (as shown below)illustrate the main effects on the liquidus (and possibly even the solidus) of the alloy as the gold content changes. As the liquidus increases, so does the tendency of the alloy to "freeze-in"voids; that is, rather than voids being able to shrink as their internal pressure decreases and reach their natural minimum size as the solder solidifies at the eutectic point, they are trapped within the solidifying alloyat alarger size.

Phase diagram of AuSn alloy showing temperature versus %w/w tin, with liquidus and solidus lines.

The obvious way tomaintain the weight ratio of tin (Sn) to gold (Au) at1:4 is by either minimizing the amount of gold on the metallizations, or by adjusting the tin content of the solder used, so that the eutectic is achieved in the final solder joint.

One way of thinking about this is the ratio of all gold in the metallizations, versus the thickness of the solder. If the solder is a preform at a 1:1 area ratio to the surfaces to be joined, then it is the thickness of the preform (see below). This is the "Gold Layer Ratio".

Diagram showing the gold layer ratio formula (a + b) / z for a solder joint between an upper.

Using this approach, the Gold Layer Ratio can be usedtoguide you to the best "off-eutectic" gold-tin alloy to minimize voiding in gold-tin eutectic solder joints, using the alloy and metal densities as a guide to building a simple model for solder joint formation, as shown below.

Chart of Au-Sn off-eutectic gold-tin solder alloys showing Au weight percent versus gold layer.

For example if you have a 0.2micron (200nm) thick layer of gold on top of nickel/tungsten as a die metallization, and a 0.4mm (400nm) layer of gold on nickel as a substrate metallization, with a 15micron thick gold/tin preform, the gold ratio is 0.04. This would suggest that a preform made at the Au79Sn21 off-eutectic would be the best choice to minimize voiding.

These alloys, usually at 1.0% increments (AuSn21, AuSn22), are available in preform, wire, sphere, and solder paste forms, and are, of course, slightly lower in cost than the standard AuSn20 alloys due to the reduced gold content.

Please let us know how we can help you meet your soldering needs!